我的博客列表

2013年4月18日星期四

Tungsten-Copper-Machining

The principal Tungsten/Copper alloys contain from 2% to 45% copper by weight. The addition of copper increases the thermal conductivity of the alloy while reducing the hardness and modulus of rupture.
The machining and grinding characteristics of tungsten/copper alloys are similar to those of hard grey cast iron. Being non-porous, standard water soluble coolants may be used if desired, but are not required. Each machine shop usually has its individual machining or grinding practice and, therefore, the information presented should be considered as a guide only.
Carballoy, grade 883 or equivalent. Grind tools with 0 deg. rake, 8-12 deg. clearance, and .010" to .025" nose radius. The nose radius can increase with the size of the work. For fine finish, stone small flat on tool parallel to work. Suggest resting stone on work when honing tool.
Roughing, approximately .030" deep and .020" per revolution feed. Finishing, .002" to.005" depth of cut and .001" to .002" per revolution feed. Turning speed, 300-500 surface feet per minute. Do not use lubricant or coolant.

没有评论:

发表评论